Vent: tried laying block wet vs dry in 95 degree heat in Phoenix, one way won big
Last week I had a small retaining wall job in Phoenix and decided to test something. I laid the first 30 blocks with dry mortar mix straight from the bag, then did the next 30 with a slightly wetter mix I let sit for 10 minutes. The wet batch stuck way better, no crumbling at the head joints, and I only had to tap each block twice instead of fighting it. Dry mix made me waste 20 minutes redoing 6 blocks that shifted. Has anyone else messed with letting their mortar slack up a bit in the heat, or am I late to this?