That folded piece of scrap plate I tacked in as a heat shield on the tube sheet, and my warp dropped to almost nothing
I fought a 60 inch waterwall panel for two and a half weeks last month and kept getting about 3/16 inch of bow at the center no matter how I sequenced my passes. Tried flipping the panel, moving my root in tighter, even preheated the whole thing, nothing worked. Out of pure aggravation one Friday I tacked a scrap piece of 1/2 plate behind the seam to pull some heat away from the back side, and the next panel came out dead flat within 1/16. Been doing it on every panel since and it costs me maybe 15 minutes of fit-up for a way better finished piece. Curious if you all are shielding heat with backing plate on panels like this or if I just got lucky on that one.